A131 DH36 | A131 grade DH36 STEEL PLATE
2011年11月15日 by admin
A131 DH36 STEEL PLATE
Gangsteel is specialized in supplying A131 high strength steel plate in A131 Grade DH36. For more information of GradeDH36 steel plate, please check them in following:
A131 DH36 high Strength Chemical Composition | |||||||
Grade | The Element Max (%) | ||||||
C | Si | Mn | P | S | Al | N | |
A131 DH36 | 0.18 | 0.1-0.50 | 0.90-1.6 | 0.035 | 0.035 | 0.015 | |
Nb | V | Ti | Cu | Cr | Ni | Mo | |
0.02-0.05 | 0.05-0.10 | 0.02 | 0.35 | 0.2 | 0.4 | 0.08 |
Crack Sensitivity: Pcm = (C+Si/30+Mn/20+Cu/20+Ni/60+Cr/20+Mo/15+V/10+5B)%
Carbon Equivalent: Ceq = 【C+Mn/6+(Cr+Mo+V)/5+(Ni+Cu)/15】%
Carbon Equivalent: Ceq = 【C+Mn/6+(Cr+Mo+V)/5+(Ni+Cu)/15】%
A131 DH36 high strength property | |||||||
Grade | | Mechanical Property | Charpy V Impact Test | ||||
Thickness | Yield | Tensile | Elongation | Degree | Energy 1 | Energy 2 | |
A131 DH36 | mm | Min Mpa | Mpa | Min % | -20 | J | J |
t≤50 | 355 | 490-620 | 22% | 17 | 25 | ||
50<t≤70 | 355 | 490-620 | 22% | 20 | 30 | ||
70<t≤100 | 355 | 490-620 | 22% | 25 | 37 | ||
Note: Energy 1 is transverse impact test, Energy 2 is longitudinal |
Equivalent steel grade of A131 DH36 | |||||||
NV D36 | GL-D36 | LR/DH36 | BV/DH36 | CCS/D36 | K D36 | R D36 | RI/D36 |