Gangsteel is specialized S355G7+M, S355G7+M is a structural grade steel supplied to the offshore industry. The material can be delivered as normalized (N) or thermo-mechanically rolled (M). Supplied in accordance with EN10225:2001, the steel offers good tensile and yield strength. 

 

S355G7+M  Chemical Composition

Grade

The Element Max (%)

C

Si

Mn

P

S

Al

N

S355G7+M

0.14

0.15-0.55

1.0-0.01

0.02

0.01

0.0055

0.01

Nb

V

Ti

Cu

Cr

Ni

Mo

0.04

0.06

0.025

0.3

0.25

0.5

0.08

Crack Sensitivity:  Pcm = (C+Si/30+Mn/20+Cu/20+Ni/60+Cr/20+Mo/15+V/10+5B)%
Carbon Equivalent:  Ceq =
C+Mn/6+(Cr+Mo+V)/5+(Ni+Cu)/15%

 

S355G7+M high strength property

Grade

 

Mechanical Property

Charpy V Impact Test

Thickness

Yield

Tensile

Elongation

Degree

Energy 1

Energy 2

S355G7+M

mm

Min Mpa

Mpa

Min  %

-40

J

J

t≤50

355

470-630

22%

50

50

50t≤63

355

470-630

22%

50

50

63t≤100

325

490-630

22%

50

50

Note: Energy 1 is transverse impact test, Energy 2 is longitudinal

 

Boiler steel plates | Alloy steel plates | High strength plate| Carbon steel plate | Stainless steel plate

 

To find out more about S355G7+M offshore steel plate, and to receive a competitive quotation for supply of this material, please CLICL HERE to contact us.  

 

 

Tags: S355G7M  EN 10225 S355G7M  EN 10225 steel plate  

0 Comments, 0 Trackbacks