New Products /back


S275ML EN10025-4 S275ML steel

2011年4月5日 by admin

EN10025-4,S275ML,S275ML steel,S275ML steel grade,S275ML steel plate.

 

Adopt Standard EN10025-4

Gang steel Grade:

EN10025-4

S275M

S275ML

S355M

S355ML

Grade

S420M

S420ML

S460M

S460ML

 

S275ML steel plate

S275ML Grade is a technical delivery conditions for thermo mechanical rolled weldable fine grain structural steels.
S means the structural steel, M means the delivery condition.
Capital letter L for the quality with specified minimum values of values of impact energy at temperature not lower than -50 degree.

 

Gangsteel is a large agent of HBIS wuyang mill in China and we are specialized in super thick S275ML steel plate. We could supply the min order is a piece and promise the competitive price in order to enlarge our oversea market.

S275ML Chemical composition of the product analysis for thermo mechanical rolled steel

Element

S275ML  Max %

Element

S275ML max %

C

0.15

AL

    0.015 min

Si

0.55

TI

0.06

Mn

1.60

CR

0.35

P

0.030

NI

0.35

S

0.025

Mo

0.13

Nb

0.06

Cu

0.60

V

0.10

N

0.017

 

S275ML Mechanical properties at ambient temperature for thermo mechanical rolled steel

Grade

Thickness

Yield Strength

Tensile Strength

Elongation

Impact Energy

(mm)

MPa (min)

MPa

% (min)

(KV J) (min)

 

 

 

 

-50 degree

S275ML

≤ 16

275

370-530

24

27

16> to ≤40

    265

370-530

24

27

40> to ≤63

255

350-510

24

27

63> to ≤80

245

350-510

24

27

80> to ≤100

245

350-510

24

27

100> to ≤120

240

350-510

24

27

 

If you want to find our stock in S275ML, or inquiry S275ML from our Gangsteel, please feel free to contact us by email or calling.

EN10025-4,S275ML,S275ML steel,S275ML steel grade,S275ML steel plate.

 

 