New Products /back


EN 10028-2 P355GH boiler and pressure vessel steel plate

2013年9月11日 by admin

EN 10028-2 P355GH steel plate

 

Related Grade:P235GH,P265GH,P295GH,p355gh,16Mo3,18MnMo4-5,20MnMoNi4-5,15NiCuMoNb5-6-4,20MnMoNi4-5,15NiCuMoNb5-6-4,13CrMo4-5,13CrMoSi5-5,10CrMo9-10,12CrMo9-10,X12CrMo5,13CrMoV9-10,12CrMoV12-10,X10CrMoVNb9-1.

 

P355GH steel grade is one of grade in En10028-2, which is non alloy and alloy steels with specified elevated temperature properties.

 

In accordance with en10020, P235GH,P265GH, P295GH and p355gh are non alloy quality steels. All of other grade are alloy special steels.

 

P355GH Grade delivery condition is normalizing or be replaced with normalizing rolling at the discretion of manufactures. 

 

Gangsteel could supply P355GH steel grade in super thick steel plate for fabricators serving the oil and gas industry, heat exchangers, weldable pressure vessels and boilers

 

Steel ServicesCutting, Painting, Pretreatment, Ultrasonic Test, Third Party Inspection, HIC, NACE, and so on.


P355GH Chemical composition cast analysis

Element

P355GH  Max %

Element

P355GH max %

C

0.08-0.20

Cr

0.30

Si

0.40

Cu

0.30

Mn

0.90-1.50

Mo

0.08

P

0.025

Nb

0.020

S

0.015

Ni

0.30

AL

0.020 min

Ti

0.30

N

0.012

V

0.02


 

P355GH Mechanical properties 

Grade

Condition

Thickness

Yield Strength

Tensile Strength

Elongation

Impact Energy

(mm)

MPa (min)

MPa

% (min)

(KV J) (min)

 

 

 

 

-20 degree

P355GH

Normalized

≤ 16

355

510-650

20

27

16> to ≤40

   345

510-650

20

27

40> to ≤60

335

510-650

20

27

60> to ≤100

315

490-630

20

27

100> to ≤150

295

480-630

20

27

150> to ≤250

280

470-630

20

27


 

If you want to find our stock in P355GH or inquiry from our gangsteel, please feel free to contact us by email or calling.

Yours sincerely,

 

Ms. Olina

Henan Gang Iron and Steel Co., Ltd

Tel: 86-0371-88884766  

Fax: 86-0371-88884766

Cell: 86-15226033579

Email: olina@gangsteel.com

Skype: gangsteel18

Tags: EN 10028-2 P355GH  P355GH  P295GH  P355GH steel plate  P355GH price  EN 10028-2  

0 Comments, 0 Trackbacks